Natisni

logo

Designation by Standards

Steel No. DIN EN AISI JIS ГОСТ
1.4742 X10CrAl18 † X10CrAlSi18 - SUS21 15Ch18SJu


Chemical Composition (in weight %)

C Si Mn Cr Mo Ni V W Others
max. 0.12 1.05 max. 1.00 18.00 - - - - Al=0.95


Description
Heat resistant steel for temperatures up to 1000oC, exposed to lower mechanical stressed structural parts.

Applications
Furnance fittings, conveying parts, components for thermal boilers, etc.

Physical properties (avarage values) at ambient temperature
Modulus of elasticity [103 x N/mm2]: Approx. 200
Density [g/cm3]: Approx. 7.7
Thermal conductivity [W/m.K]: 19.0
Electric resistivity [Ohm mm2/m]: 0.95
Specific heat capacity[J/g.K]: 0.45
Magnetisable: Yes

Coefficient of Linear Thermal Expansion 10-6 oC-1

20-200oC 20-400oC 20-600oC 20-800oC 20-1000oC
13.0 13.5 14.5 15.0 15.5


Annealing
Heat to 800-850oC.

Mechanical properties at at ambient temperature
Condition: Annealed
Hardness: max. 212 HB
0.2% proof stress: 270 N/mm2
Tensile strength: 500-700 N/mm2
Elongation: min. 12%

1% Creep Stress Limit in N/mm2 vs. Temperature in oC

600oC 700oC 800oC 900oC 1000oC
27.5 8.5 3.7 1.8 0.7


Forging
Hot forming temperature: 1100-800oC.

Machinability
No data.

Remark
All technical information is for reference only.